Masterbatch COL 8125 TPU black
Uniform Black Coloring of TPU with COL 8125 TPU Black
The COL 8125 TPU black masterbatch uses a polyester-TPU carrier instead of PP or PE. With a pigment content of 35% and a recommended dosage of 1–2%, it provides ideal conditions for uniform black coloring and high-quality surfaces.
The choice of carrier material is critical for TPU coloring
A black masterbatch based on a PP or PE carrier introduces a polyolefin phase into the material that is chemically different from the TPU. Depending on the TPU type, dosage, and processing conditions, this can lead to uneven distribution, varying black depth, or surface defects. For demanding applications, the suitability of the carrier material should therefore be verified.
Possible defects when using a PP or PE carrier
Marbling, streaks, or gray areas; a washed-out appearance of the black color or uneven black depth; specks and grainy surface defects; as well as color variations between batches. These defects can occur in particular when the masterbatch carrier material does not disperse sufficiently in the TPU.
What Masterbatch COL 8125 TPU black offers
The pigment is embedded in a polyester-TPU matrix and thus in a carrier from the same polymer family as the material to be colored. No PP or PE carrier is introduced via the masterbatch.
This choice of carrier creates more favorable conditions for uniform pigment distribution. The goals are to achieve a homogeneous black color and to reduce surface defects.
TPU processing guidelines highlight the risk of incompatibilities with unsuitable carrier materials.
Applications:
- Injection molding
- Extrusion
- Films
- Profiles
- Cables
- Flexible technical components
PP or PE carriers compared to TPU carriers
| Criterion | Masterbatch based on PP or PE carriers | Masterbatch COL 8125 TPU black |
| Carrier material | Polyolefin; chemically distinct from TPU | Polyester-TPU |
| Pigment distribution | Depends on the compatibility of the two matrices | A TPU substrate promotes uniform distribution |
| Color consistency | Risk of marbling and uneven black density | Promotes uniform black coloration |
| Surface quality | Defects possible if compatibility is insufficient | More favorable conditions due to the TPU substrate |
| Composition of the component | Additional introduction of PP or PE via the carrier | No introduction of a PP or PE carrier |
Four steps to your first processing test
Drying
Pre-dry the TPU and masterbatch separately. For the masterbatch, dry for 3 hours at 70 °C. For the TPU, follow the drying specifications provided by the respective manufacturer.
Dosing
Start with a dosage of 1% and gradually increase it to up to 2%, depending on the part thickness, desired opacity, and blackness.
Comparison
Conduct the test on the same machine, using the same mold or extrusion die, and with the same settings as those used with the previously employed masterbatch. Change only the masterbatch.
Approval
For components with critical requirements, verify that the properties specified in the specifications are met after coloring.
Request a Sample
We would be happy to provide you with a sample so you can evaluate the color, pigment distribution, and material behavior under your processing conditions.
To select a suitable sample, we need the following information:
- TPU type and exact material designation: polyester or polyether
- Shore hardness;
- Processing method: injection molding, extrusion, etc.
Contact us now—our team will be happy to assist you!
Product Profile
- Product Type: Black masterbatch on a polyester-TPU carrier base
- Form: Free-flowing granules
- Pigment content: 35%
- Recommended dosage: 1–2%
- Calculated pigment content in the mixture:
Approx. 0.35% with a 1%
masterbatch addition; approx. 0.70% with a 2% addition - Temperature resistance: Up to 200 °C
- Lightfastness: Specified value: 7–8
- Pre-drying: 3 hours at 70 °C
- Storage: Store in a cool, dry place in the original packaging
- Shelf life: At least 12 months from shipment